# 12 — Field testing and fakes: what each test can and cannot prove

**Order: non-destructive tests first. Never acid-test, file or tap someone else's merchandise without explicit permission** (C08). Every test below has false positives and false negatives. Conclusions should read "consistent with…", not "confirmed".

## 1. Aisle sequence
1. **Look:** overall form, seams, wear-through color at edges, felt bases, glass liners.
2. **Loupe the marks** (10×) under raking light, and transcribe them exactly (05–08).
3. **Magnet:** body, rim, handle, foot and fittings each separately.
4. **Weigh** (0.1 g scale) and compare with size and the calibration tables (02, 03).
5. **Decide.** Leave destructive tests until after purchase, or ask first.

## 2. Test-by-test

| Test | Physical basis | False result to expect | Verdict |
|---|---|---|---|
| **Magnet** | Silver is diamagnetic (NIST, C08) | **Passes but not silver:** copper, brass, nickel silver, lead, pewter, Britannia metal, plate on these, and annealed 304/316 stainless. **Sticks but is silver:** a steel blade, spring, rod or screw in a sterling piece | Screens out iron and steel only. Report "no ferrous core at tested points" [S52](https://assistwithbuying.com/guides/silver/99-sources#s52) |
| **Marks** | A claim by the maker | Forged or transposed punches, "925" struck on plate or pewter, pseudo-hallmarks | Evidence, not proof (§3) |
| **Heft** | Sterling 10.36 g/cm³ vs copper 8.94, zinc 7.14, lead 11.34 | Weighted pieces feel heavy; hollow sterling feels light | Clue only |
| **Ping / ring** | Resonance depends on geometry and damping | Shape dominates; there is no universal "silver sound" | Do not rely on it. Risks damage |
| **Ice melt** | Silver conducts heat at 429 W/m·K | Copper (≈400) passes; thin silver fails | Do not rely on it |
| **Bleach** | Silver chloride forms | Plate reacts too; it damages the surface | **Never** |
| **Cloth / chalk "smudge"** | Silver sulfide tarnish | Plate tarnishes too; lacquered sterling leaves no mark | Do not rely on it |
| **Bite / bend** | Softness | Lead and pewter are soft too; it damages the item | **Never** |
| **Acid (commercial kit)** | Reagent color compared against standards | Face of plated items reads "silver"; solder spots mislead | Destructive; owner's consent only |
| **Specific gravity** | Archimedes | Fails on hollow, weighted, stone-set or glass-mounted items | Good for solid homogeneous pieces |
| **Handheld XRF** | Surface element spectrum | Reads only the outer ~10–50 µm; plate can read as silver; surface enrichment overstates fineness; solder spikes Pb/Sn | Best non-destructive tool, but only a **surface** reading |
| **Fire assay** | Cupellation | — | Gold standard. Destroys the sample; used for refinery settlement |

## 3. Acid tests: reading and safety
- **Schwerter's-type silver solution** (nitric acid + potassium dichromate). Vendor scale: **bright red ≈ fine; dark red ≈ sterling; brown ≈ .800; green/blue ≈ low-silver or base metal**. Shades vary by brand and timing (G08; Medium).
- **Gold test acid on silver:** a milky or cloudy reaction suggests silver; a green fizz suggests copper or brass (G08).
- A face that reads "sterling" while a worn edge reads green means the piece is **layered or plated**. Confirming solid metal under heavy plate requires a filed notch, which is destructive.
- Use commercial kits only, never homemade acids. Work ventilated, with gloves and goggles, and follow the SDS. **US Poison Control: 1-800-222-1222** (C08).

## 4. XRF limits (High, C08/G08)
- Information depth decays exponentially. For silver it is roughly 10–15 µm in coin studies and up to 30–50 µm in some protocols.
- **ISO 23345:2021** limits ED-XRF fineness work to homogeneous items; coated items need multilayer methods such as ASTM B568 (G08; Medium).
- XRF cannot see internal fill, lead cores or steel rods.
- Curved surfaces, tarnish and short scans distort readings.

## 5. Documented fakes and look-alikes

| Look-alike | Mistaken for | Best check |
|---|---|---|
| Fine electroplate | Sterling | EPNS/EPBM or pseudo-marks; copper or brass at wear points |
| Nickel silver | Coin silver or tarnished sterling | ALPACA, NICKEL SILVER; yellow-grey tone; lower density |
| Weighted sterling | Heavy solid pieces | WEIGHTED or REINFORCED; base plug; magnet at the stem |
| Sterling-mounted glass | All-silver vessel | Inspect the collar; weigh the glass separately |
| Forged British marks | Antique sterling | The Goldsmiths' Company documents forged and **transposed** punches; Ashley-Russell fakes were undetectable from photos [S30](https://assistwithbuying.com/guides/silver/99-sources#s30) |
| Fake Native artist stamps | Native-made jewelry | DOJ 2019 and 2026 cases [S50](https://assistwithbuying.com/guides/silver/99-sources#s50). Match to documented stamps |
| Spratling and Taxco copies | Spratling originals | Match the punch to museum examples [S38](https://assistwithbuying.com/guides/silver/99b-sources#s38); TS-24 = successor work [S37](https://assistwithbuying.com/guides/silver/99b-sources#s37) |
| Silvered bronze or spelter (zinc) | Cast sterling figures | Base-metal color underneath; spelter ~7.1 g/cm³ |
| Filled bars and tourist ingots | Bullion | Dimensions and weight vs mint spec; ultrasound |
| "Acid tested" seller tags | Verified sterling | Treat as unverified; surface tests pass on plate |

## 6. Missing or odd marks
- **No mark ≠ not silver:** the US does not require marks, the UK has weight exemptions, and old pieces are often unmarked. Say "possibly silver, unverified" (C08).
- **Weak, double-struck or worn marks** are normal. Unusually crisp marks on a heavily worn piece, or marks set in a soldered panel, deserve scrutiny.

## 7. How to state a conclusion (template)
"**Classification:** sterling (marked STERLING + Gorham lion-anchor-G). **Tests:** non-magnetic at the body and foot; no wear-through. **Not tested:** acid, XRF. **Construction:** solid, no weighting seen. **Confidence:** high for solid sterling; maker attribution high."